Compound V117
Description – 75 Durometer FKM Red
Specification (specs) – ASTM D2000 M2HK810 A1-10 B38 EF31 EO78 F15, Z1
| PROPERTY | RESULT | SPECS |
|---|
| Hardness, Shore A (Type M) | 74 | 75 +/- 5 |
| Tensile Strength, Min MPa | 13.8 | 10 |
| Elongation, min % | 1.61 | 150 |
| Specific Gravity | 2.16 | Report |
A1-10 Heat Resistance 70hrs at 250C
| Hardness Change, pts max | +3 | +10 |
| Tensile Strength Change, max % | +4 | -25 |
| Elongation Change, max % | -9 | -25 |
B38 Compression Set Method B
| 22hrs at 200C, max % | 14.0 | 50.0 |
EF31 Fuel C Resistance 70hrs at 23C
| Hardness Change pts | -2 | +/- 5 |
| Tensile Strength Change, max % | -22 | -25 |
| Elongation Change, max % | +10 | -20 |
| Volume Change % max | +5 | 0 to +10 |
EO78 Fluid No 101 Resistance 70hrs at 200 C
| Hardness Change pts | -8 | -15 to +5 |
| Tensile Strength Change, max % | -22 | -40 |
| Elongation Change, max % | +10 | -20 |
| Volume Change % max | +11 | 0 to +15 |
F15 Low Temperature Resistance
| Non Brittle after 3 min @-25C | Pass | Pass |
Z1 TR10 retraction at Low temperature Resistance
| 51 mm die 50% Elongation, C | -18.0 | Report |